The choice depends on the aluminium alloy. For AlMg alloys such as 5083 and 5086, choose AlMg5 or AlMg4.5Mn. For AlMgSi alloys such as 6060 and 6082 and for casting alloys containing silicon, choose AlSi5 or AlSi12. For pure aluminium, use Al99.7.
First determine the alloy group
Aluminium falls into three groups. Pure aluminium comes in purities from 99.0 to 99.7 percent. Non-heat-treatable alloys contain small amounts of manganese or magnesium, with AlMg alloys containing up to 5 percent magnesium being common. Heat-treatable alloys contain copper, magnesium with silicon, or zinc with magnesium.
Pure aluminium and most non-heat-treatable and heat-treatable alloys are readily weldable. With heat-treatable alloys containing copper, however, there is a risk of hot cracking, which makes them difficult to weld. Casting alloys with a high copper or magnesium content are not always weldable either. So determine in advance which alloy you are dealing with.
The range at a glance
Product AWS Material number Typical application Al99.7 A5.10 approx. ER1100 3.0259 Pure aluminium, tanks and sheet metal work AlSi5 A5.10 ER 4043 3.2245 AlMgSi alloys, thin-walled work, frames AlSi12 A5.10 ER 4047 3.2585 Casting alloys up to 12 percent silicon, heat exchangers AlMg4.5Mn A5.10 ER 5183 3.3548 5083, pressure vessels, tanks for liquefied gas AlMg5 A5.10 ER 5356 3.3556 5086, 5454, 6061, shipbuilding and transport For most combinations of base materials, AlMg5 and AlSi5 are the starting point. If the component comes into contact with seawater or sea air, the AlMg grades are preferred because of their corrosion resistance.
MIG or TIG
The two dominant processes for aluminium are MIG and TIG. TIG is the better choice for thin-walled material, when there are requirements for the appearance of the weld, for single-sided welding such as on pipes, and for repair work. TIG welding of aluminium is usually done on alternating current. Use MIG for thicker materials and when speed matters in combination with long continuous welds.
There are also versions for gas welding and for welding with covered electrodes. You will find these under brazing rods and stick electrodes.
Where aluminium is used
- Shipbuilding, in particular yachts, smaller vessels and specialised ships
- Tanks and bodywork in transport and vehicle construction
- Heat exchangers and pressure vessels
- Repair of castings such as cylinder heads and pump housings
Points of attention with aluminium
- Remove the oxide layer just before welding, as it melts at a much higher temperature than the aluminium beneath it
- Take the high thermal conductivity into account, you need more heat input than for steel of the same thickness
- Aluminium does not change colour when heated, which makes burn-through difficult to see
- Work cleanly and use a separate set of tools for aluminium
For welding pure aluminium and casting alloys in repair work, Al99.7 is also available as a TIG rod. For components that will be anodised, the choice of filler metal affects the colour after anodising. Mention this in your enquiry and we will take it into account in our advice.
The complete data sheets and safety data sheets can be found under aluminium documentation.