How do I weld cast iron?

Cast iron is cold welded with a nickel-based electrode. For grey and malleable cast iron, use HILCO Pure Nickel; for all cast iron grades including nodular cast iron and for heavy, restrained parts, use HILCO Nickel Iron.

Why cast iron requires special attention

Enormous quantities of components are cast, because casting is the most economical way of making machine parts. Cast iron is by nature somewhat brittle. Its structure tends to break rather than deform under a hard blow. That makes it vulnerable in service, but fortunately it can be repaired well.

Matching welding is not possible here. Instead, you use a nickel-based filler metal that produces tough, crack-resistant weld metal that is easy to machine. This way, you restore the component without new cracks forming.

The choice between the two products

Cast iron gradeFirst choiceSecond choice
Grey cast ironPure NickelNickel Iron
Nodular cast ironNickel IronPure Nickel
Malleable cast ironNickel IronOn request
Cast iron to steelNickel IronPure Nickel
ProductAWSCharacter
Pure NickelA5.15 E Ni-CIPure nickel weld metal, approx. 97.5 percent nickel, easy to machine
Nickel IronA5.15 E Ni Fe-CITough nickel-iron weld metal, high crack resistance

Pure Nickel is suitable for cold welding grey and malleable cast iron and for joining these materials to steel, copper and copper alloys. The product can also be used on heavily contaminated castings. Nickel Iron is suitable for all common cast iron grades, including phosphorus-containing cast iron, and is the choice for heavy sections and highly restrained parts.

Practical points of attention

  • Clean the surface thoroughly, oil and dirt penetrate porous cast iron
  • Weld with short beads and allow the workpiece to cool in between
  • With cast iron, maintain an interpass temperature of approximately 60 degrees Celsius to limit thermal stress
  • Peening the weld metal helps to reduce welding stress
  • Both electrodes are supplied vacuum packed, so that they stay dry until use

Where you will come across this

Pumps, engine parts, machine housings and bearing blocks are often made of cast iron. This is common on ships, because there are many pumps on board to move liquids. The same applies to drives and machine parts in factories.

When the cast iron grade is unknown

If you cannot establish which cast iron grade is involved, Nickel Iron is the safer choice, because the product can be used on all common grades. If it is even unclear whether the material is cast iron or steel, but it is certain that the material is ferrous, you can fall back on Hilchrome 312R. That is an emergency solution and not a replacement for proper material identification.

Pure Nickel is also used as a buffer layer. You first apply a layer of pure nickel and then continue filling with Nickel Iron. That combination works well on heavily contaminated castings or castings that are difficult to assess.

A more detailed discussion can be found under welding of cast iron.

In doubt about the cast iron grade? Contact us for advice on the approach.

Contact

Do you have a question? Feel free to contact us using this contact form!

  1. What is hardfacing and when do you apply it?
    "

    Hardfacing is the application of a wear-resistant weld layer to a component so that it lasts longer. You apply it to components that become thinner due to abrasion, impact or friction, and you apply it to worn components or preventively to new components.

    How it works in practice

    Compare it to a knife that becomes blunt and thinner through frequent use. You apply a number of weld layers, grind them back to size and the component is usable again. The same happens with a roller that crushes sugar cane. At a certain point, the roller has worn down so far that it no longer meets the tolerances and the product is no longer fully crushed. The roller is dismantled, a few centimetres of material are built up by welding, and it is machined flat again on the lathe. It then goes back into production.

    This is not a one-off repair but an ongoing process. In many companies it is simply part of the maintenance schedule, for example twice a year. The component is not replaced, it is maintained.

    The three steps of restoration

    StepWhat you doWhy
    Buffer layerApply an intermediate layerDilutes the carbon and alloy content of the base material
    Build-upRestore heavily worn parts to sizeRestores the original dimensions with crack-resistant material
    HardfacingApply the wear-resistant top layerProtects the surface against further wear

    Not every repair requires all three steps. With light wear, you can hardface directly. With crack-sensitive base material, a buffer layer is recommended. Hilchrome 312R is a commonly used choice for this.

    Where you will come across hardfacing

    • Earthmoving machinery, buckets and teeth in mining
    • Ploughs, harvesting machines and planting machines in agriculture
    • Rollers, filters and piping in the sugar industry
    • Conveying and processing installations in the cement industry
    • Pumps, mixers and valves in the process industry

    In agriculture and earthmoving, a specific form of wear is added. Components that move through soil, sand and stones are subject to abrasive wear. On stony or volcanic ground this happens faster than in soft clay, but it occurs everywhere.

    The benefit for your operations

    The key issue is downtime. If a component breaks and you have to wait until a new one has been shipped, flown in or even manufactured from scratch, production is at a standstill in the meantime. If the component can be removed, repaired and refitted, the downtime is a fraction of that time.

    In addition, you extend the service life of existing components. In this way, a machine gets a second and sometimes a multiple life. From a sustainability perspective, that is interesting: the component is reused after restoration, instead of being scrapped and replaced.

    Read more about this in our article repair instead of replacing for less downtime and a longer service life and on our repair and maintenance page.

    We are happy to help you choose the right hardfacing product for your wear situation.

    "
  2. Which hardfacing product should I choose for which type of wear?
    "

    The choice depends on the type of wear. For abrasive wear with impact, choose HILCO Hardmelt 600, for heavy abrasion with moderate impact Hardmelt 638, and for sliding wear with heavy impact Hardmelt 620. If you work with wire, HILCO H-600 and HILCO Hilcord 600 are the counterparts.

    First determine the type of wear

    Wear occurs in different forms, and these call for different solutions. Look at what actually happens to the component in practice and what function it has.

    • Metal to metal, with rolling or sliding parts with little lubrication
    • Heavy impact, where the surface is crushed or cracks
    • Abrasion combined with impact, with granular material under impact loading
    • Heavy abrasion, where granular material grinds the surface away
    • Metal to soil, with earth and sand and moderate impact
    • Corrosion, where chemical attack plays a role

    The range per situation

    Wear situationCovered electrodeWire
    Moderate abrasion, high impactHardmelt 600H-600 or Hilcord 600
    Heavy abrasion, moderate impactHardmelt 638On request
    Sliding wear, heavy impactHardmelt 620H-600
    Sliding wear with corrosionHilchrome 312R or 307ROn request
    Buffer layer before hardfacingHilchrome 312ROn request

    The technical data

    ProductClassificationHardnessSpecial feature
    Hardmelt 600DIN 8555 E 6-UM-60approx. 600 HBBasic coated, for steel, cast steel and high manganese steel
    Hardmelt 620AWS A5.13 E Fe 5-B mod.See data sheetRutile coated, up to approx. 550 degrees Celsius
    Hardmelt 638EN 14700 E Z Fe14See data sheetHigh efficiency, 205 percent recovery
    H-600EN 14700 S Fe8approx. 600 HBSolid wire, martensitic structure
    Hilcord 600DIN 8555 MSG 6-GF-60-GPapprox. 600 HBSeamless metal-cored wire

    The weld metal of these products is martensitic and so hard that it can only be finished by grinding. Turning or milling is not possible. Take this into account in your work preparation.

    Points of attention when welding

    • Preheat crack-sensitive base materials and apply a buffer layer first
    • Monitor the interpass temperature in accordance with the instructions on the data sheet
    • Determine in advance how many layers are needed to return to the original dimensions
    • Bear in mind that the last layer is the wear-resistant layer

    Electrode or wire

    Both forms are used side by side in practice, and that has to do with the workplace. If the component is treated in a workshop, you work with wire. That is a continuous process without the interruptions that occur with electrodes, which makes a big difference on larger surfaces. If the component has to be repaired in the field, for example a machine that cannot be brought indoors during the season, you use an electrode because gas shielding does not work there.

    The same installation therefore sometimes requires both versions. A factory repairs the rollers and internal components indoors with wire, and the machines that work outdoors with electrodes.

    The classification according to EN 14700 is explained under classification EN 14700. The data sheets can be found under repair and maintenance documentation.

    Describe the wear situation and the base material, and we will advise you on the build-up of the weld layers.

    "
  3. How do I weld cast iron?
    "

    Cast iron is cold welded with a nickel-based electrode. For grey and malleable cast iron, use HILCO Pure Nickel; for all cast iron grades including nodular cast iron and for heavy, restrained parts, use HILCO Nickel Iron.

    Why cast iron requires special attention

    Enormous quantities of components are cast, because casting is the most economical way of making machine parts. Cast iron is by nature somewhat brittle. Its structure tends to break rather than deform under a hard blow. That makes it vulnerable in service, but fortunately it can be repaired well.

    Matching welding is not possible here. Instead, you use a nickel-based filler metal that produces tough, crack-resistant weld metal that is easy to machine. This way, you restore the component without new cracks forming.

    The choice between the two products

    Cast iron gradeFirst choiceSecond choice
    Grey cast ironPure NickelNickel Iron
    Nodular cast ironNickel IronPure Nickel
    Malleable cast ironNickel IronOn request
    Cast iron to steelNickel IronPure Nickel
    ProductAWSCharacter
    Pure NickelA5.15 E Ni-CIPure nickel weld metal, approx. 97.5 percent nickel, easy to machine
    Nickel IronA5.15 E Ni Fe-CITough nickel-iron weld metal, high crack resistance

    Pure Nickel is suitable for cold welding grey and malleable cast iron and for joining these materials to steel, copper and copper alloys. The product can also be used on heavily contaminated castings. Nickel Iron is suitable for all common cast iron grades, including phosphorus-containing cast iron, and is the choice for heavy sections and highly restrained parts.

    Practical points of attention

    • Clean the surface thoroughly, oil and dirt penetrate porous cast iron
    • Weld with short beads and allow the workpiece to cool in between
    • With cast iron, maintain an interpass temperature of approximately 60 degrees Celsius to limit thermal stress
    • Peening the weld metal helps to reduce welding stress
    • Both electrodes are supplied vacuum packed, so that they stay dry until use

    Where you will come across this

    Pumps, engine parts, machine housings and bearing blocks are often made of cast iron. This is common on ships, because there are many pumps on board to move liquids. The same applies to drives and machine parts in factories.

    When the cast iron grade is unknown

    If you cannot establish which cast iron grade is involved, Nickel Iron is the safer choice, because the product can be used on all common grades. If it is even unclear whether the material is cast iron or steel, but it is certain that the material is ferrous, you can fall back on Hilchrome 312R. That is an emergency solution and not a replacement for proper material identification.

    Pure Nickel is also used as a buffer layer. You first apply a layer of pure nickel and then continue filling with Nickel Iron. That combination works well on heavily contaminated castings or castings that are difficult to assess.

    A more detailed discussion can be found under welding of cast iron.

    In doubt about the cast iron grade? Contact us for advice on the approach.

    "
  4. Why does hardness alone say nothing about wear resistance?
    "

    Two products can state the same hardness and yet differ greatly in service life. Hardness says something about the resistance to indentation, not about the resistance to wear. What matters is the way in which that hardness is achieved.

    Two routes to the same hardness

    You can achieve hardness by adding a lot of carbon. Carbon is inexpensive and produces a high value on the measuring scale. You can also achieve the same hardness by adding molybdenum and chromium. These are more expensive alloying elements, but they create a fine-grained structure that is considerably more resistant to wear at the same hardness.

    On paper, the same number appears in both cases. In practice, one product lasts longer than the other. Anyone who only looks at the stated hardness is therefore not comparing what they think they are comparing.

    How to compare instead

    What to look atWhy it matters
    The chemical compositionShows which alloying elements build up the hardness
    The structure of the weld metalA martensitic structure performs differently from a high carbon content
    The classification according to EN 14700 or DIN 8555Indicates the field of application, not just the hardness
    The type of wear it is intended forAbrasion, impact and friction each require different properties
    The number of maintenance interventions per yearThe practical measure of what a product delivers

    The chemical composition of our products is stated on the data sheet. For critical applications, we also supply a quality certificate with the measured values per batch. This allows you to compare on the data that really matter.

    The calculation that counts

    Suppose you have to hardface a component twice a year with product A and once a year with product B. Then product B may cost more per kilo and you will still be better off at the end of the year. Moreover, one fewer maintenance intervention also means one fewer shutdown of the installation.

    So do not only look at the price per kilo, but at what the product delivers in your situation over a maintenance cycle. This applies in particular to repair and maintenance, where the frequency of intervention determines the real costs.

    What we do and do not claim

    We do not make general statements about the service life of our products compared with those of others. What we do is demonstrate what our products consist of and which values we have measured. On that basis, you can make a substantiated comparison yourself. For the associated documentation, please refer to material test certificates.

    Would you like to see the composition of a specific hardfacing product? Contact us and we will send you the data sheet.

    "
Certificates
  • TUV.png
  • LR.png
  • ISO.png
  • DNV.png
  • CE.png
  • Bureau Veritas.png
  • AEO.png
  • ABS.png
Read more >
Receive our newsletter!

Sign up for the free newsletter to stay up to date

Quotation Shopping cart

Your shopping cart is still empty!

Add products from the catalog to place an order
Continue shopping
  • :
  • :
  • Total weight
Op voorraad
Not in stock
excl. VAT
Aanbevolen producten